Green part, brown part, sintered part: the ceramic process chain

A ceramic part passes through three states before it is ceramic. Each has its own rules.

30 October 20266 min ReadCeramics
Ceramic pellets as feedstock for pellet-based 3D printing

In plastics printing a part is finished when the printer stops. In technical ceramics that is where the work begins. The part passes through three states, each with its own name, its own properties and its own failure modes – and once you know them, you design differently from the outset.

State 1: the green part

What comes off the printer is called the green part. It consists of ceramic powder bound in a polymer matrix and already resembles the finished part – only larger. It can be handled, transported and even machined.

That machinability is why printing ceramics pays off against grinding from solid: in the green state the material is soft enough for conventional tools. What would later take diamond tooling and hours takes minutes now. There is more on this in printing technical ceramics instead of grinding them.

The green part is more delicate than it looks. Wall thicknesses below 0.8 millimetres rarely survive the steps that follow.

State 2: the brown part

Debinding drives the polymer matrix out. What remains is a body of pure ceramic powder, held together only by its own packing density – the brown part, named after the discolouration that occurs as the binder is removed.

This is the most critical moment in the whole chain. The brown part has barely any strength; one careless grip is enough. At the same time, this is where it is decided whether the part gets any further at all: if debinding runs too fast, the part tears open from the inside because the escaping gases find no way out. That is why every material and every wall thickness needs its own programme.

We carry out debinding and sintering in house. That shortens the feedback loop considerably when a part does not make it through first time – we do not have to wait for a service provider before adjusting the schedule.

State 3: the sintered part

In the furnace the powder particles bond, the voids between them close and the part densifies to 98 to 99 per cent of theoretical density – shrinking as it does so. Only now does it have the properties ceramics are chosen for in the first place: hardness, temperature resistance, chemical resistance.

What exactly happens in the furnace, and why shrinkage is a design matter, is covered in sintering ceramics.

What this means for your design

StatePropertyTypical risk
Green partmachinable, oversizedwalls too thin, breakage during handling
Brown partvery fragile, purely ceramiccracks if debinding runs too fast
Sintered partdense, hard, near net shapedistortion from uneven wall thicknesses

All three risks have the same root: uneven distribution of material. Design even wall thicknesses, keep to at least 0.8 millimetres and build solid sections above 15 millimetres with a low infill, and you have avoided the main pitfalls.

Radii, by contrast, are uncritical – here you have more freedom than in many other processes. It gets harder where a lot of support material would be needed, because in pellet-based printing the material can only be retracted to a limited extent.